this post was submitted on 04 Sep 2023
46 points (92.6% liked)

3DPrinting

15130 readers
18 users here now

3DPrinting is a place where makers of all skill levels and walks of life can learn about and discuss 3D printing and development of 3D printed parts and devices.

The r/functionalprint community is now located at: [email protected] or [email protected]

There are CAD communities available at: [email protected] or [email protected]

Rules

If you need an easy way to host pictures, https://catbox.moe may be an option. Be ethical about what you post and donate if you are able or use this a lot. It is just an individual hosting content, not a company. The image embedding syntax for Lemmy is ![](URL)

Moderation policy: Light, mostly invisible

founded 1 year ago
MODERATORS
 

I was printing a benchy on my monoprice select miniwitha a e3d v6 nockoff and I saw plastic ozzing around my hotend

you are viewing a single comment's thread
view the rest of the comments
[–] [email protected] 23 points 11 months ago (1 children)

In my experience the hole that the thermistor goes into isn’t in the path of the filament. So probably what’s happening is either the nozzle or the tube that screws into the other side of the heater block is loose, allowing melted plastic to escape through a place other than the tip of the nozzle.

After you’ve cleaned it out, what I like to do before running filament through again is to turn the hot end on, let it come up to temp, then tighten the nozzle a bit more. The joint expands when heated so even if you’ve got it right at room temp it can still need tightening at the working temperature.

[–] [email protected] 9 points 11 months ago

This is definitely the right answer, as I just had to deal with this after a nozzle change.